材料性能 / 工程材料库
35CrMo Class.螺柱 (≤M22) 最小Sy=735 [GB/T 150.2 2024]
返回材料列表
材料标准
GB/T 150.2 2024
(表E.7)
弹性模量E (GPa)
| 温度(℃) |
值 |
| 20.00 |
201.0000 |
| 100.00 |
197.0000 |
| 150.00 |
194.0000 |
| 200.00 |
191.0000 |
| 250.00 |
188.0000 |
| 300.00 |
183.0000 |
| 350.00 |
178.0000 |
| 400.00 |
170.0000 |
| 450.00 |
160.0000 |
| 500.00 |
149.0000 |
热膨胀系数TE (10-6m/m℃)
| 温度(℃) |
值 |
| 0.00 |
10.7600 |
| 50.00 |
11.1200 |
| 100.00 |
11.5300 |
| 150.00 |
11.8800 |
| 200.00 |
12.2500 |
| 250.00 |
12.5600 |
| 300.00 |
12.9000 |
| 350.00 |
13.2400 |
| 400.00 |
13.5800 |
| 450.00 |
13.9300 |
| 500.00 |
14.2200 |
| 550.00 |
14.4200 |
| 600.00 |
14.6200 |
设计应力强度Sm (MPa)
| 温度(℃) |
值 |
| 20.00 |
210.0000 |
| 100.00 |
190.0000 |
| 150.00 |
185.0000 |
| 200.00 |
179.0000 |
| 250.00 |
176.0000 |
| 300.00 |
174.0000 |
| 350.00 |
165.0000 |
| 400.00 |
154.0000 |
| 425.00 |
147.0000 |
| 450.00 |
140.0000 |
| 475.00 |
111.0000 |
| 500.00 |
79.0000 |
屈服强度Sy (MPa)
| 温度(℃) |
值 |
| 20.00 |
735.0000 |
| 100.00 |
665.0000 |
| 150.00 |
645.0000 |
| 200.00 |
625.0000 |
| 250.00 |
615.0000 |
| 300.00 |
605.0000 |
| 350.00 |
580.0000 |
| 400.00 |
540.0000 |
| 450.00 |
490.0000 |